A note that says "general tolerances ISO 8062-3 CT8" does not give one tolerance. It gives a table: the grade names the column, the feature's nominal size picks the row, and the cell is the total band the casting may use. A 20 mm feature and a 300 mm feature on the same CT8 drawing do not get the same number, and neither gets a single ± value without halving.
Most tolerance arguments start because one side read the grade as a promise and the other read it as a table. Here is the table, the extra allowances that hide behind it, and the three questions that separate a capable quote from a copied note.
For ductile and gray iron in machine-produced sand moulds, ISO 8062 practice centers on CT8 to CT12. The values below are the total tolerance bands for CT8 and CT9 as published by a working foundry for machine-molded ductile and malleable iron sand castings.
| Nominal size, mm | CT8 | CT9 |
|---|---|---|
| up to 10 | 1.0 | 1.5 |
| 10–16 | 1.1 | 1.6 |
| 16–25 | 1.2 | 1.7 |
| 25–40 | 1.3 | 1.8 |
| 40–63 | 1.4 | 2.0 |
| 63–100 | 1.6 | 2.2 |
| 100–160 | 1.8 | 2.5 |
| 160–250 | 2.0 | 2.8 |
| 250–400 | 2.2 | 3.2 |
| 400–630 | 2.6 | 3.6 |
Fill in the coarser grades from the same pattern: each grade step widens the band by roughly 40 percent, and every row widens with size. The geometric growth is the point. Pattern expansion, mould wall movement and solidification shrinkage do not scale down with feature size, which is why ±0.5 mm is routine on a 25 mm feature and physically optimistic on a 400 mm one.
Process maps onto grade roughly like this: CT4–CT6 belongs to investment casting and die casting; CT7–CT9 is what a controlled machine-molded sand line delivers; CT10–CT12 covers hand molding, large castings and difficult geometry. A supplier who quotes CT6 on a 200 kg sand casting either copied your note back or has not measured the process. Either answer deserves a question before the order, not after the first rejection.
The CT band does not travel alone. Three add-ons live next to it, and drawings that ignore them generate rejections nobody can fix.
Mismatch is the first. Features that cross the parting line inherit the alignment error between cope and drag — around 0.7 mm on machine-molded work, more on hand molding. It is not added to the CT band; it sits beside it as a separate allowance the drawing has to declare. A bore centered 30 mm from the parting line does not care. A bore straddling the line does.
Draft is the second. Vertical faces need draft to pull from the sand, typically 1–2 degrees for pattern work. A dimension measured across a drafted face changes with the height at which it is measured, and ISO 8062 does not absorb that into CT.
Machining allowance, RMA, is the third and the expensive one. ISO 8062-3 defines RMA per size and machining method; in practice, a sand-cast ductile face destined for machining carries 2–4 mm of stock, more on large faces that can warp. The stock has to swallow the full CT band plus the mismatch plus the distortion the heat treatment will add — a normalized casting moves after its dimensional report is taken. If the RMA is sized only against nominal CT, machining will find skin.
Newer drawings carry DCTG grades — required casting tolerance grades — instead of a blanket CT note. The distinction is practical. CT describes what a process achieves; DCTG tells the foundry which features genuinely need it.
The economical drawing does three things. It sets a general DCTG that the process can hold without heroics — DCTG 8–10 on machine-molded ductile iron. It tightens only the features that mate, locate or seal, usually a handful. And it marks datum pads that survive to machining, because every machined feature inherits the position error of the datum it references. Blanket-tightening a whole casting to CT7 buys nothing but price.
Which grade do you hold on this size band, not on your best part? Capability drifts with size; a foundry that holds CT8 up to 50 kg and CT9 above is telling the truth. One that claims CT8 everywhere has probably not measured.
Show me the scatter, not the pass. A first-article report with pass marks proves one part. A dimensional report with actual values across twenty parts from several moulds proves a process. If the readings cluster within a third of the band, the capability is real.
Do the numbers include heat treatment? A casting that gets stress-relieved, normalized or austempered changes after the furnace. The dimensional report that matters is the one taken after the last thermal step and before machining.
Our DISA vertical line and shell process carry the usual CT8–CT9 on machine-molded work, CT10–CT12 on hand molding and large pieces, and we publish which band applies to each size class rather than quoting one number everywhere. When a drawing arrives with a general note tighter than the process can hold across its size, we quote the grade we can hold and list the features that need machining instead — that conversation costs ten minutes and saves rework either way.
We also flag dimensions that cross the parting line, dimensions that depend on core position, and any drawing that mixes as-cast and post-heat-treatment dimensions without saying which is which. Those three notes on the quote are not disclaimers; they are the difference between a tolerance that inspection can verify and one that starts arguments.
What does CT8 mean in plain numbers?
It depends on the feature size. On a 50 mm feature it is a 1.4 mm total band, or roughly ±0.7 mm. On a 400 mm feature the same grade is 2.2 mm total. The grade names the column; the size picks the row.
Is CT7 achievable in sand casting?
On small features from a well-controlled machine-molded line, on a first article, sometimes. Across a production run and a size range, CT8–CT9 is the honest band for ductile iron in sand. Anything tighter is usually a machining job, not a casting promise.
What is the difference between CT and DCTG?
CT is what a process achieves; DCTG is what the drawing requires, per feature if needed. Newer drawings use DCTG so that critical features get a tight grade without forcing the whole casting to pay for it.
Do I need to state mismatch separately?
For any dimension that crosses the parting line, yes. The mismatch allowance sits outside the CT band, around 0.7 mm on machine-molded moulds, and the drawing should declare it or accept it in the RMA.
Why did my castings move after heat treatment?
Thermal cycles release residual stress and shift sections at different rates. Measure dimensions after the last thermal step. A report taken as-cast does not describe a normalized part.
How much machining stock should I allow?
Enough to swallow the CT band, the mismatch, and heat-treatment movement — 2–4 mm on a machined face is the usual sand-casting band, more on large faces. Undersized RMA is the most common cause of "skin on the machined face" claims.
Send the drawing with the general grade, the tightened features marked, the parting line location, and the machining surfaces with their stock expectations. We will return the grade we hold per size class, the mismatch allowance that applies, and the RMA per machined face — so the tolerance conversation ends before the pattern starts, where changes are free.
Related reading: ductile iron casting properties and grade data, how to audit a casting supplier before the first order, our foundry process and capacity, and gray iron properties by grade.